Skip to main content

Blog

Ultrasonic Welding: Weak Welds, Surface Marks, and When Not to Raise Amplitude or Energy

A weak ultrasonic weld with surface scorching, whitening or a through-weld is not a reason to raise amplitude or energy first. Check the horn face, trigger, hold and joint feature before changing those settings.

Published 2026-11-28 · SHNEHP

A weak ultrasonic weld that already shows surface scorching, whitening or a hole through the wall is not a reason to raise amplitude or weld energy first. Those changes put more motion and more heat into the same contact path. They do not seat a horn that is only touching on one edge, and they do not rebuild a joint feature that was never there.

This note is about that pairing of a weak joint and a damaged surface on a small part. It is not a frequency-selection discussion, and not a design comparison of energy directors and shear joints.

The marks often appear before the joint has really worked

Design examples: a small appliance housing, or an electronics cover that closes a shallow molded base. These are structural examples, not delivered machines or customer parts.

Ultrasonic welding converts electrical energy into high-frequency mechanical vibration. The horn applies that vibration and pressure to the joint. Localized frictional heat fuses the plastic. When the vibration stops, the material cools under pressure. The public product page describes this route for small and medium thermoplastic parts, without adhesive or an external heat source.

On the cover example the horn is close to the seam, so the usual question is how that energy enters the part, not a lack of amplitude. If the working face is worn, dirty or tilted, the high spot on the cosmetic surface takes the motion first and the joint under it may barely melt. Raising the setting then marks that surface more deeply, and can punch through a thin cover, while the weld stays patchy.

When not to raise amplitude or energy

Leave the settings alone and inspect the contact path first.

The horn is not sitting on the intended face. A tilted stack, a worn or dirty working face, or a cover that only meets the horn on a rib or a logo will leave a bright mark or a white blush in that spot. More energy goes into the same high point.

Vibration starts at the wrong moment. If it starts before the horn has settled, the face can skate and scuff the surface. If it starts so late that the cover is already crushed, the joint may be closed mechanically and still not welded. Neither case is corrected by a higher energy value.

The hold after vibration stops is not keeping the melt in place. The public description is clear that the plastic has to cool under pressure. If the horn lifts too soon, or the fixture lets the cover spring back, extra melt runs out as flash. A larger energy input only makes that flash heavier.

The joint feature does not match the part. A cover may need a continuous energy director or a shear engagement, and arrive with a crushed director, a mismatched groove, or a flat face where that feature should have been. More amplitude heats whatever is already touching. It will not rebuild the feature.

The surface is already scorched, white, or locally welded through. At that point the cosmetic face has taken more than it can accept. Raising amplitude or energy usually makes the mark, the hole or the flash worse. It is not a repair step.

This is not a promise that a particular amplitude or energy value will correct the next lot. The contact path and the joint have to be able to use the setting first.

Check the horn face, the trigger, the hold and the joint first

A practical order is to look at what already touched the part, then at the settings.

Inspect the working face of the horn and the surface it meets. Clean or redress the face if it is marked or contaminated. Confirm that the fixture supports the joint from behind, so the cover cannot dish away from the horn. Before the cycle starts, load both halves and check that the director or shear feature is present, continuous and opposite its mating face.

Watch when vibration begins relative to contact, and whether the horn stays down long enough for the melt to freeze. If the cover already shows a scorch, a white mark or a through-weld, treat that as a limit, not as a prompt to add more energy.

Only after the horn sits evenly, the joint feature is actually working, and a short trial no longer damages the surface does it make sense to compare amplitude or energy. If the weld is still weak, go back to those checks rather than adding more motion.

SHNEHP builds ultrasonic welding machines around the part, the joint and the tooling. Send the housing or cover, the marks you already see and the joint layout, so contact and settings can be reviewed together.

Websites: shnehp.com | shnehp.cn

Request a Technical Consultation

Send your part drawing, sample information, plastic material and target cycle time. Our engineers will recommend a practical hot plate welding machine configuration.