Skip to main content

Blog

Plastic Pallet Welding: Short Rib Welds, Deck Sag, and When Not to Raise Plate Temperature or Heat Time

If pallet rib welds look closed but the deck still sags, or flatness gets worse after welding, do not raise hot-plate temperature or heat time first. Check rib contact, support and cooling set.

Published 2026-11-28 · SHNEHP

A double-deck plastic pallet can leave the station with rib welds that look closed, and still sag under load, or sit less flat than the molded halves. That is not a reason to raise the hot-plate temperature or extend the heating time first. More heat softens a larger volume of plastic. It does not put a short rib onto its mating face, or hold a deck that was never supported through cooling.

The subject here is short rib welds and deck sag after the cycle, not a station-by-station account of how a pallet is welded, and not a model-selection note.

A closed perimeter can still leave the deck without enough support

Design example: a heavy-duty double-deck pallet in HDPE or PP, with a separately molded top deck and bottom base. This is a structural example, not a delivered machine or a customer part.

Pallet welding machines use a large-format hot plate to join the two halves into a hollow-box structure. A heated platen melts the internal ribs and the perimeter mating surfaces. The platen retracts, and the machine presses the halves together so the melt can freeze, as the public product page describes. What the deck will carry depends on which ribs actually met, and on whether the deck was held while the melt set.

On this example the perimeter may already look continuous. A finger along the outer seam can find no gap, yet the internal ribs are what keep the deck from dishing between the edges. If some ribs were short, poorly seated, or melted away before their neighbors made contact, the deck can still sag between the ribs that did weld. Raising plate temperature, or leaving the halves on the platen longer, makes more melt at the ribs already touching. Those ribs can collapse further, and the short ones still never arrive.

When not to raise plate temperature or heat time

Stop and look at contact, support and cooling first.

The ribs and their mating faces were never opposite each other. A layout that drops a rib into a cavity, a warped deck from molding, or a nest that seats the half on the wrong feature will start the heat step with a gap already built in. Extra heat does not stretch a short rib across that gap.

Some ribs reach the platen early, and others never do. The early ribs then carry the heat and the later press. If they are already slumped, adding temperature or time usually slumps them more, and the deck follows them down.

The tooling does not support the deck through the press and the cool. Once the ribs are soft, a thin deck takes the shape of whatever is under it. If support is only at the corners, or the halves are released before the melt has set, more heat leaves more soft material to sag.

Cooling and set are uneven, or cut short. The extra heat then stays in the deck, and flatness can get worse after the pallet leaves the station, even if the seams looked acceptable in the tool.

The pallet already shows collapsed ribs, heavy flash, a dished deck, or a twist that was not in the molded halves. More plate temperature or a longer heat time is usually an aggravation, not a repair.

This is not a promise that a particular temperature or heating time will correct the next pallet. The heat step helps only after the ribs can meet and the deck is held until the melt is solid.

Check layout, rib contact, support and cooling set first

Look at the rib path before changing the heat.

Lay the planned welds on the top and bottom decks over one another and see which internal ribs have a mating face. Load both halves in the tools, without asking the platen to make up a gap, and check that the load-bearing ribs are already able to meet. Confirm that the nest supports those ribs and the field of the deck during the press and through cooling.

If a trial pallet already sags, find the short or collapsed ribs under the low area rather than asking the plate to run hotter. A welded-looking perimeter does not prove a continuous rib structure underneath.

Only after the ribs stay in contact and the deck is held through set does it make sense to compare plate temperature or heat time. If the deck still sags, or flatness is worse than the incoming halves, go back to layout, support and cooling.

SHNEHP supplies pallet welding machines and large-format tooling for top and bottom decks. If a trial pallet already sags or shows short ribs, send the deck and rib layout with the sag location, not a request to run the plate hotter.

Websites: shnehp.com | shnehp.cn

Request a Technical Consultation

Send your part drawing, sample information, plastic material and target cycle time. Our engineers will recommend a practical hot plate welding machine configuration.